论文部分内容阅读
耐候钢S355J2(/%:0.07~0.12C,0.25~0.40Si,1.0~1.3Mn,≤0.015P,≤0.008S,0.25~0.40Cu,0.35~0.50Cr,0.10~0.25Ni,0.025~0.040Nb,0.025~0.050Als)的冶炼流程为70 t LD-LF-VD-280 mm×320 mm坯CC工艺。通过控制LD终点[C]≤0.07%,终点[P]≤0.014%,转炉下渣量≤2 kg/t和LF精炼渣碱度R≥3.0,(Al_2O_3)=20%等工艺措施,铸坯的T[O]为