【摘 要】
:
我厂为了贯彻“压力容器安全监察规则”,对碱性焊条进行400℃以上烘干,购进了8810型电热鼓风干燥箱。但在使用半年左右,风扇轴和电动机轴的联轴器就损坏了,按原样修复不久就
【机 构】
:
常州化工机械厂焊试室,常州化工机械厂焊试室,常州化工机械厂焊试室,
论文部分内容阅读
我厂为了贯彻“压力容器安全监察规则”,对碱性焊条进行400℃以上烘干,购进了8810型电热鼓风干燥箱。但在使用半年左右,风扇轴和电动机轴的联轴器就损坏了,按原样修复不久就又坏了。经分析其原因认为:主要是因烘箱是用薄钢板制成,刚度较差,在经400℃以上温度烘烤一段时间后,内部有所变形,这样就加大了轴与轴之间的不同心度,造成风叶
I plant in order to implement the “pressure vessel safety supervision rules”, alkaline electrode above 400 ℃ drying, purchased the 8810 electric blast oven. However, after about six months of use, the coupling of the fan shaft and the motor shaft was damaged, and the original repair was broken shortly afterwards. The analysis of the reasons that: mainly because the oven is made of thin steel plate, the stiffness is poor, after baking at a temperature above 400 ℃ for some time, the internal deformation, thus increasing the difference between the shaft and the shaft Heart, resulting in leaves
其他文献
介绍沥青混凝土路面病害出现的原因,并提出了根治的方法。
Describes the causes of asphalt concrete pavement disease and puts forward the radical method.
本法除抗坏血酸钼兰法的基本原理处,利用高酸度提高五价砷的氧化电位,以溴化钾为还原的动力催化剂,亚硫酸钠-硫代硫酸钠(简称“双硫”)为砷与铁的复合还原剂为特点,使砷还原
S195汽缸盖是缸径为95毫米单缸卧式柴油机的重要零件。铸件重9.4公斤。平均壁厚8毫米左右。材质为HT20—40。柴油机工作时,汽缸盖壁部内外温差大,热应力大,因此对机械性能有
改装前,395M磨床的主轴运动,是由棉织皮带将电机动力,通过四个区紧轮传动到砂轮轴上。由于砂轮滑板的上下移动,使压紧轮来回摆动,因此砂轮轴受到振动,使磨削光洁度只能达8,而
球化处理工艺,目前国内有铁水冲入法、合金坨压入法,压力加镁法等。从1980年开始,国外有些工厂先后采用盖包处理法,因有其独特优点,国外采用此方法进行球化处理的工厂愈来愈
我厂汽轮机辅机抽气系统中的收缩管(如图1所示),由于工作时内腔受到空气或水的冲刷,要求光洁,无铸造缺陷和一定的气密性。该零件采用ZQAL9—2铝锰青铜铸造,由于该合金的收缩
温挤压是一种少无切削工艺,从七十年代开始,在国内陆续用于生产。在连续生产中,采用温挤加工时,由于坯料温度较高,使模具的温度也较高,导致了模具的强度、硬度降低,寿命受到
一引言我厂是以铜冶炼为主的多品种综合有色企业,年耗标准煤7万吨左右。十一届三中全会以来,品种又有了较大发展,增设了黄铜带生产线,但一些费能型设备依然被采用。几年来对
与往事可以干杯,但积淀的历史传统智慧必须要继承。古典的理解因为文字和教育的断裂,让现代国人颇费脑筋。因而,稀有的可以解读古典的学者的作品对于我们理解古典思想似乎就
骨髓增生异常综合征(MDS)是一种起源于造血干细胞的克隆性疾病,疾病临床表现呈异质性,多数患者最终转化为急性髓细胞性白血病。近年来发现DNA甲基化异常与MDS的严重程度及预