一、前言 电冲转的混合工艺,不但解决了转炉落渣引起回磷;降低脱硫效果的问题。而且电冲转时渣温高,渣流动性好,生产调度方便,化学成分稳定等优点,从大连钢厂试验的结果来看,脱硫率,脱氧率,钢中夹杂,钢中气体,低倍和机械性能都达到了电炉钢的水平。这种混合工艺,对我国电炉一般在5~15吨,转炉一般在6~12吨来说,是切实可行的。 I. INTRODUCTION Electro-impulse mixing process not only solves the problems of phosphorus removal caused by slag drop in converter, but also reduces desulfurization effect. In addition, the slag temperature is high, the slag fluidity is good, the production scheduling is convenient and the chemical composition is stable. According to the test results of the Dalian steel mill, the desulfurization rate, the deoxidation rate, the inclusions in the steel, the gas in the steel, And the mechanical properties have reached the level of EAF steel. This mixing process, the electric furnace in China is generally 5 to 15 tons, the converter is generally 6 to 12 tons, it is feasible.
其他文献
上钢五厂转炉炉衬工段创造了转炉快速砌炉和快速拆炉的经验。使停炉到开炉的时间由原需的50~60小时缩短到22小时,其主要的经验为: (1)快速砌炉: 1)劳动组织的改善: 两个砌炉
本文论述了使用喷射法,用无镁稀土合金作球化剂处理不同含硫量的铁水制备球墨铸铁的可能性。喷射法由于改善了球化反应动力学条件,稀土和镁一样是优良的球化剂。文中对稀土球
吹氩可以净化钢质。顶吹氩优于底吹氩。沸腾钢和一般镇静钢采用吹氮代替吹氩,将显著提高钢的质量。喷吹硅钙粉2公斤/吨,脱硫效率一般达70~90%,[O]在20ppm以下时,[S]可以脱到小
近年来,地方骨干钢铁企业继续贯彻执行国民经济调整方针,加强了能源管理,针对本企业的薄弱环节,采取了一系列有效的节能措施,即使在煤、电供应紧张的不利条件下,能耗仍继续
江西钢厂1983年进行了转炉优钢化工作,转炉冶炼20管用钢7534.94吨,质量达到了电炉钢的水平。钢的含氮量仅为电炉钢的36%,钢中夹杂物总量与电炉钢相当。又由于采用了钢包吹氩
安徽省合肥财贸钢厂以革命的首创精神,在0.2吨转炉上试验成功了用石灰石作为转炉炉衬材料。炉龄一般都在100炉以上,最高达到181炉的全国最高记录。这是转炉炉衬中的一个新事
自83年3月份以后,我厂18米~2烧结机在运转中台车偏向轨道一侧的现象日趋显著。南边台车轮缘在3号吸风箱后就与钢轨紧密贴合,此后台车就一直严重地啃轨运行,轮缘和钢轨内侧相
秦皇岛冶金机修总厂是以制造热风阀为主的专业生产厂。产品行销全国各省、市钢铁和化工企业,目前生产的品种有:φ500、φ700、φ900、φ1100热风阀和各种杂阀,包括冷风阀、
由有色金属分析情报网举办的《稀土总量化学分析经验交流会》于1984年9月18日至22日在包头市举行。包头冶金研究所及上海跃龙化工厂共同主持了会议。来自18个省市自治区的39